TYPICAL MAGNETIC PERFORMANCE OF CAST ALNICO MAGNETS |
Equivalent
MMPA Class |
Grade |
Br |
Hcb |
(BH)max |
%ChangePer¡æ |
Tc |
Tw(Max) |
Density |
mT |
Gs |
KA/m |
Oe |
KJ/m3 |
MGOe |
Br |
Hcj |
¡æ |
¡æ |
G/cm3 |
AlNiC03 |
LN9 |
680 |
6800 |
37 |
470 |
9 |
1.13 |
-0.03 |
-0.02 |
760 |
450 |
6.9 |
LN10 |
600 |
6000 |
40 |
500 |
10 |
1.25 |
-0.03 |
-0.02 |
760 |
450 |
6.9 |
AlNiCo2 |
LNG12 |
700 |
7000 |
45 |
565 |
12 |
1.50 |
-0.03 |
-0.02 |
810 |
450 |
7.0 |
LNG13 |
680 |
6800 |
48 |
600 |
13 |
1.60 |
-0.03 |
-0.02 |
810 |
450 |
7.0 |
AlNiCo5 |
LNG34 |
1180 |
11800 |
48 |
600 |
34 |
4.30 |
-0.02 |
0.02 |
890 |
525 |
7.3 |
LNG37 |
1200 |
12000 |
48 |
600 |
37 |
4.65 |
-0.02 |
0.02 |
890 |
525 |
7.3 |
LNG40 |
1220 |
12200 |
48 |
600 |
40 |
5.00 |
-0.02 |
0.02 |
890 |
525 |
7.3 |
LNG44 |
1250 |
12500 |
52 |
650 |
44 |
5.50 |
-0.02 |
0.02 |
890 |
525 |
7.3 |
AlNiCo5DG |
LNG52 |
1300 |
13000 |
55 |
690 |
52 |
6.50 |
-0.02 |
0.02 |
890 |
525 |
7.3 |
AlNiCo5--7 |
LNG60 |
1300 |
13000 |
58 |
725 |
60 |
7.50 |
-0.02 |
0.02 |
890 |
525 |
7.3 |
AlNiCo6 |
LNGT28 |
1050 |
10500 |
56 |
700 |
28 |
3.50 |
-0.02 |
0.03 |
860 |
525 |
7.3 |
AlNiCo7 |
LNGT18 |
580 |
5800 |
90 |
1130 |
18 |
2.20 |
-0.03 |
0.02 |
860 |
550 |
7.3 |
AlNiCo8 |
LNGT32 |
800 |
8000 |
104 |
1300 |
32 |
4.00 |
-0.03 |
0.02 |
860 |
550 |
7.3 |
LNGT38 |
800 |
8000 |
110 |
1380 |
38 |
4.75 |
-0.03 |
0.02 |
860 |
550 |
7.3 |
LNGT40 |
820 |
8200 |
110 |
1380 |
40 |
5.00 |
-0.03 |
0.02 |
860 |
550 |
7.3 |
AlNiCo8HC |
LNGT36J |
700 |
7000 |
140 |
1750 |
36 |
4.50 |
-0.03 |
0.02 |
860 |
550 |
7.3 |
AlNiCo9 |
LNGT60 |
900 |
9000 |
110 |
1380 |
60 |
7.50 |
-0.03 |
0.02 |
860 |
550 |
7.3 |
LNGT72 |
1050 |
10500 |
112 |
1410 |
72 |
9.00 |
-0.03 |
0.02 |
860 |
550 |
7.3 |
|
| |
TYPICAL MAGNETIC PERFORMANCE OF SINTERED ALNICO MAGNETS |
| |
Equivalent
MMPA Class |
Grade |
Br |
Hcb |
(BH)max |
¦Á(Br) |
Tc |
Tw(Max) |
Density |
mT |
Gs |
KA/m |
Oe |
KJ/m3 |
MGOe |
%/¡æ |
¡æ |
¡æ |
G/cm3 |
S.Alnico 3 |
FLN8 |
550 |
5500 |
42 |
530 |
9.0 |
1.13 |
-0.022 |
760 |
450 |
6.7 |
S.Alnico 2 |
FFLNG12 |
700 |
7000 |
48 |
600 |
12.4 |
1.55 |
-0.014 |
810 |
450 |
7.0 |
S.Alnico 7 |
FFLNGT18 |
580 |
5800 |
90 |
1130 |
18.0 |
2.20 |
-0.020 |
850 |
500 |
7.2 |
S.Alnico 5 |
FLNG34 |
1100 |
11000 |
48 |
600 |
34.0 |
4.25 |
-0.016 |
890 |
500 |
7.2 |
S.Alnico 6 |
FLNGT28 |
1000 |
10000 |
56 |
700 |
28.0 |
3.50 |
-0.020 |
850 |
500 |
7.2 |
S.Alnico 8 |
FLNGT38 |
800 |
8000 |
100 |
1250 |
32.0 |
4.00 |
-0.020 |
850 |
500 |
7.2 |
FLNGT42 |
850 |
8500 |
110 |
1380 |
38.0 |
4.75 |
-0.020 |
850 |
500 |
7.2 |
S.Alnico 8HC |
FLNGT33J |
680 |
6800 |
140 |
1750 |
36.0 |
4.50 |
-0.025 |
850 |
500 |
7.2 |
|
| |
TYPICAL MAGNETIC PERFORMANCE OF BONDED ALNICO MAGNETS |
| |
Grade |
Br |
Hcb |
Hcj |
(BH)max |
¦Á(Br) |
Tc |
Tw(Max) |
Density |
mT |
Gs |
KA/m |
Oe |
KA/m |
Oe |
KJ/m3 |
MGOe |
%/¡æ |
¡æ |
¡æ |
G/cm3 |
BA-A |
300 |
3000 |
88 |
1100 |
112 |
1400 |
6 |
0.8 |
-0.02 |
760 |
180 |
5.6¡ª5.8 |
BA-B |
350 |
3500 |
80 |
1000 |
103 |
1300 |
8 |
1.0 |
-0.02 |
760 |
180 |
|
|
|