SmCo magnet is high magnetic performance and low temperature coefficient. Its b iggest advantage is superior resistance to high temperature. It needn't to be coa ted because it is difficult to be eroded and oxidized. >SmCo magnet is widely used in motors, watch, transducers, instruments, meters, positiona detector, generators, aviation, spaceflight and radar, etc. |
|
|
|
TYPICAL MAGNETIC PERFORMANCE OF SINTERED SMCO MAGNETS |
| Grade |
Br |
Hcb |
Hcj |
(BH)max |
¦Á(Br) |
Tc |
Tw(Max) |
Density |
ALLOY |
| mT |
Gs |
KA/m |
Oe |
KA/m |
Oe |
KJ/m3 |
MGOe |
%/¡æ |
¡æ |
¡æ |
G/cm3 |
SERIES |
| SC18 |
840 |
8400 |
605 |
7600 |
1432 |
18000 |
143 |
18 |
-0.04 |
750 |
250 |
8.0-8.2 |
SmCo5 |
| SC20 |
890 |
8900 |
637 |
8000 |
1432 |
18000 |
159 |
20 |
-0.04 |
750 |
250 |
8.0-8.2 |
| SC22 |
930 |
9300 |
637 |
8000 |
1432 |
18000 |
175 |
22 |
-0.03 |
750 |
280 |
8.3-8.5 |
Sm2Co17 |
| SC24 |
980 |
9800 |
676 |
8500 |
1432 |
18000 |
191 |
24 |
-0.03 |
800 |
280 |
8.3-8.5 |
| SC24H |
980 |
9800 |
676 |
8500 |
1989 |
25000 |
191 |
24 |
-0.03 |
800 |
330 |
8.3-8.5 |
| SC26L |
1030 |
10300 |
398 |
5000 |
438 |
5500 |
207 |
26 |
-0.03 |
800 |
180 |
8.3-8.5 |
| SC26 |
1030 |
10300 |
716 |
9000 |
1194 |
15000 |
207 |
26 |
-0.03 |
800 |
250 |
8.3-8.5 |
| SC26M |
1030 |
10300 |
716 |
9000 |
1592 |
20000 |
207 |
26 |
-0.03 |
800 |
300 |
8.3-8.5 |
| SC26H |
1030 |
10300 |
716 |
9000 |
1989 |
25000 |
207 |
26 |
-0.03 |
800 |
330 |
8.3-8.5 |
| SC28L |
1070 |
10700 |
398 |
5000 |
438 |
5500 |
223 |
28 |
-0.03 |
800 |
180 |
8.3-8.5 |
| SC28 |
1070 |
10700 |
756 |
9500 |
1194 |
15000 |
223 |
28 |
-0.03 |
800 |
250 |
8.3-8.5 |
| SC28M |
1070 |
10700 |
756 |
9500 |
1592 |
20000 |
223 |
28 |
-0.03 |
800 |
300 |
8.3-8.5 |
| SC30L |
1100 |
11000 |
398 |
5000 |
438 |
5500 |
239 |
30 |
-0.03 |
800 |
180 |
8.3-8.5 |
| SC30 |
1100 |
11000 |
772 |
9700 |
1194 |
15000 |
239 |
30 |
-0.03 |
800 |
250 |
8.3-8.5 |
| SC30M |
1100 |
11000 |
772 |
9700 |
1592 |
20000 |
239 |
30 |
-0.03 |
800 |
300 |
8.3-8.5 |
TYPICAL MAGNETIC PERFORMANCE OF BONDED SMCO MAGNETS
| Grade |
Br |
Hcb |
Hcj |
(BH)max |
¦Á(Br) |
Tc |
Tw(Max) |
Density |
| mT |
Gs |
KA/m |
Oe |
KA/m |
Oe |
KJ/m3 |
MGOe |
%/¡æ |
¡æ |
¡æ |
G/cm3 |
| BS-4 |
400 |
4000 |
278 |
3500 |
800 |
10000 |
32 |
4.0 |
-0.08 |
720 |
120 |
6.2¡ª6.5 |
| BS-6 |
500 |
5000 |
318 |
4000 |
800 |
10000 |
48 |
6.0 |
-0.08 |
720 |
120 |
| BS-8 |
600 |
6000 |
318 |
4000 |
800 |
10000 |
64 |
8.0 |
-0.08 |
720 |
120 |
| BS-10L |
700 |
7000 |
318 |
4000 |
400 |
5000 |
80 |
10.0 |
-0.08 |
720 |
100 |
| BS-10 |
700 |
7000 |
398 |
5000 |
800 |
10000 |
80 |
10.0 |
-0.08 |
720 |